Board repair is not the place for guesswork.

Every seasoned SMT process engineer has at least one nightmare story about bad rework chemistry. Whether it’s the wrong flux sneaking into the operation, underprocessed flux remaining on the board or improper residue removal, they all risk the same inglorious fate: field failure. While rework operators and process engineers rarely get a glimpse of the long-term damage of inappropriate materials or processes, the failure analysis engineers see it all. They report that the vast majority of solder-related issues are on reworked solder joints, and the lion’s share of those is due to the rework chemistry.

How does the wrong flux work its way into rework? Simple human error. In some cases, operators who experience difficulty using approved rework fluxes on parts with poor solderability bring in more active materials from their personal collections. In auditing rework stations, we’ve found all sorts of unapproved soldering fluxes, including tubes of wire from electronics hobby stores (once with zinc alloy solder!), plumbing flux, and even stained glass flux. Fluxes meant for non-electronic applications are highly active and are corrosive failures just waiting to happen.

Speaking of corrosive failures waiting to happen, we can recall situations in which organic acid flux, which absolutely must be cleaned, appeared in operations that were 100% no-clean. In one case, a warehouse mix-up shipped the wrong cored wire, and it slipped into production one spool at a time for several weeks, affecting thousands of assemblies before the mistake was discovered. In another case, the term “organic” was erroneously selected by an environmentally minded buyer who assumed it would be a more eco-friendly product.

These well-intentioned, honest mistakes aren’t 100% guarded against or tested for in any size operation; they can happen in large companies and small, low-cost and high, domestic or offshore. No one is immune, so the best defense is diligence in operator education and regular auditing.

Even the right fluxes can cause reliability problems if not processed properly. Proper processing means adequate heat exposure and/or post-soldering cleaning. No-clean fluxes require heat to activate them. If processed properly, they typically pose no reliability threat and can remain on the PCB for the life of the product. But if they don’t see enough heat, dangerous levels of ionic materials may remain. With the simple additions of a voltage bias and atmospheric moisture, those unspent activators can begin attacking all the metals in the system: the solder, the component leads, and the PCB copper. Figure 1 shows an example of a corrosive failure. This type of failure can also occur if no-clean fluxes are not cleaned properly.



Partially cleaning a no-clean flux residue is worse than not cleaning it at all. The safest way to use a no-clean rework flux is to leave the residues intact to do their job. Insulative materials are designed into the fluxes and tested for electrical reliability. Partially removing flux residues can strip away the protective materials and expose the ionic compounds that attack the metals. Figure 2 shows the white, powdery “puddle” left behind after incomplete cleaning and/or rinsing.



If cleaning is necessary, solvent choice is critical. IPA is one of the most common – and most ineffective – cleaning solvents. Depending on the flux chemistry, IPA is one of those solvents that may only partially dissolve the residues. Solvents that are specifically designed to dissolve flux are a much better choice than IPA, although IPA does serve as a good, fast-drying rinse agent.

In any cleaning operation, pre- or post-rework, matching the solvent to the soil is critical. Figure 3 shows the visible effects of mismatched solvent and rework flux.
Many one-step flux removal solvents are available that do not require rinsing. These aerosol products are selected based on their chemical compatibility with specific types of flux residues, but a myriad of other factors like safety and process compatibility can drive performance tradeoffs and limit options.



Two rights can make a wrong. Even fluxes that are considered “safe” individually can cause reliability problems if they are used in the wrong combinations. Chemical incompatibilities between the ingredients of two or more different flux formulations can cause problems ranging from simple, harmless greening to complete, catastrophic failure.

Most rework fluxes are purchased from the same supplier as the primary attach fluxes, and many common combinations are pretested for compatibility by their supplier. But if the supplier hasn’t tested the specific combination, or if the primary attach and rework fluxes are from different suppliers, they should be tested together.

How does a process engineer prevent rework chemistry-related field failures?

The best way to ensure electrochemical reliability of reworked solder joints is to use the right flux delivery system. Typically cored wire, felt tip pen or gel, as shown in Figure 4, dispenses the flux only where heat will be applied, and leaves the no-clean residues intact. If the flux residues must be cleaned, ensure they are cleaned completely.

Karl Seelig is vice president of technology at AIM Solder; kseelig@aimsolder.com. Tim O’Neill is regional manager at AIM.

Reliability Problems from Underactivating fluxes

The oxide-reducing agents in electronics assembly fluxes are called activators. In no-clean fluxes, the activators are triggered by thermal exposure, and they are usually designed to work over a broad time-temperature window. They get spent as they react with the oxides on the PCB and components. Overactivation, or flux burnout (see our August column), is easy to spot because it immediately causes wetting problems. Underactivation is not as obvious because its effects aren’t plainly visible until corrosion sets in during use.

Underactivation can occur when:


Surface Insulation Resistance (SIR) and Rework Flux

SIR is a measurement of a flux or flux residue’s electrical resistivity. Higher SIR values typically indicate “safer,” or more electrochemically reliable fluxes, in typical service environments. SIR testing protocol is set by standards organizations like IPC or Telcordia, which dictate test methods and pass/fail criteria, including minimum resistance of the flux residue, usually 100MΩ or higher.

Because heat expends a flux’s ionic activators, fluxes processed at higher temperatures will often produce higher SIR values – and therefore be considered safer and more reliable – than fluxes processed at lower temperatures or fluxes that are not heated at all. Figure 4 shows the SIR test data for a typical wave solder flux. In its unheated state, it does not meet minimum reliability criteria, but after thermal exposure, it exceeds the criteria by several orders of magnitude.

When selecting rework fluxes, it is important to consider the actual process; most rework operations do not guarantee that all the flux dispensed on the PCB will be exposed to the same thermal excursion. A rework flux’s heat exposure can be limited by overdispensing, dispensing in the wrong location, or by spreading away from its original location. To help ensure reliability of rework fluxes: